200 t/h Granite Sand Making Line
Granite sand at 200 t/h with a two-stage VSI circuit that keeps flaky particles under 8% and fineness modulus at 2.8, for concrete and asphalt filler use.

Granite makes stronger sand than limestone and charges you for it in wear parts. At 200 t/h the difference between a well-arranged circuit and a badly arranged one shows up mostly in the flakiness index, which is what concrete producers actually reject sand for. This layout uses a vertical shaft impactor in closed circuit with a screen to keep flaky particles below 8%.
The flakiness problem
Granite is a coarse-grained rock with strong feldspar crystals. When it is broken in a cone crusher the fracture follows grain boundaries and produces flat, elongated fragments. Those fragments pack badly, raise the void ratio in concrete and force the mix designer to add cement. A VSI breaks along the crystal rather than between crystals, which is why every hard-rock sand plant finishes with one.
Process flow
Crushing to 30 mm
A PE-750x1060 jaw takes 500 mm granite down to 120 mm, followed by a HPT200 cone at 25 mm close side. Two stages before the VSI is the minimum for granite: feeding anything coarser than 40 mm into a sand maker triples its wear rate and does not improve shape.
Sand making in closed circuit
The VSI5X-9532 operates in closed circuit with a 2YKR-2160 screen. Oversize returns to the VSI, finished 0-5 mm goes to washing. The recirculating load is deliberately held at 45-55%, which is where flakiness drops below 8% without the power consumption running away.
Washing and dewatering
Granite sand carries less clay than limestone but more microfines from the crushing action. A spiral washer followed by a dewatering screen brings moisture down to 12%, which is what makes the sand shippable by tipper without turning into a solid block.
Equipment list
| Stage | Equipment | Qty | Power |
|---|---|---|---|
| Primary | PE-750x1060 jaw crusher | 1 | 110 kW |
| Secondary | HPT200 cone crusher | 1 | 160 kW |
| Sand making | VSI5X-9532 | 1 | 2 x 200 kW |
| Screening | 2YKR-2160 | 1 | 30 kW |
| Washing | XL-915 spiral washer | 1 | 22 kW |
| Dewatering | Dewatering screen | 1 | 15 kW |
Wear parts, honestly
Granite in a VSI consumes 0.8-1.1 kg of tungsten carbide tips and rotor wear plates per tonne of sand, roughly twice the limestone figure. Budget USD 0.22 per tonne for wear and set the rotor speed at 1,650 rpm rather than 1,850 — the lower speed costs 3% in throughput and buys 25% in tip life.
Questions we are asked before quoting
Can I make both sand and aggregate from the same plant?
Yes. Split the screen undersize: 40% to sand making, 60% to the aggregate stockpiles, and vary the split with the market. The plant above is arranged so the VSI can be bypassed entirely in a month when sand demand is low.
How do I control the filler content?
A dynamic classifier after the VSI. Without one, granite sand typically lands at 8-11% passing 75 microns, which is acceptable for C25 but marginal above C35.