Quartz and Feldspar Ultrafine Grinding Line
Grinding quartz and feldspar to 200-1250 mesh without picking up iron: ceramic lining, iron-free classification, and why the contamination limit decides the mill type.

Quartz and feldspar are cheap minerals sold at a high price only when they are clean. A silica powder at 99.5% SiO2 with 80 ppm Fe2O3 sells for glass and electronics; the same powder with 400 ppm iron sells for concrete. The grinding circuit is where the iron comes from, and no amount of washing afterwards removes it. Design the mill around contamination, not around throughput.
The contamination chain
Iron enters at four points, and each needs a different fix.
| Source | Contribution | Fix |
|---|---|---|
| Crusher wear parts | 150-400 ppm | Ceramic or tungsten-carbide faced jaw plates |
| Mill liners and media | 200-800 ppm | Alumina or zirconia lining, flint or ceramic media |
| Classifier and ducting | 50-150 ppm | Polyurethane or ceramic wear liners |
| Ambient air and handling | 20-80 ppm | Bag filter, enclosed conveying |
A steel-lined Ball Mill is the single largest contributor. Running quartz through it produces a powder that will never meet a glass-grade specification, however good the deposit. This is the first decision in the project.
Process flow
Feed preparation
Feed should already be washed and preferably attrition-scrubbed to remove surface staining, because surface iron on the grains goes straight into the product. A jaw crusher with ceramic-faced plates reduces it to below 20 mm. A magnetic separator ahead of the mill removes free iron from worn conveyor parts but does nothing for the iron locked in the mineral.
Grinding
Two routes. For 200-400 mesh at volume, a ball mill with alumina lining and flint or high-alumina media. For 800-1250 mesh, a stirred or ring-roll ultrafine mill with ceramic wear surfaces. The energy curve is steep: 200 mesh costs 25-35 kWh/t, 800 mesh costs 90-130 kWh/t, and 1250 mesh costs 150-200 kWh/t. If the customer wants 1250 mesh, ask what they are using it for before designing the circuit, because at that fineness the power bill often exceeds the product value.
Classification and product collection
An air classifier with a ceramic-lined rotor gives a sharp top cut and lets one mill deliver several grades by changing rotor speed. For glass-grade silica the requirement is usually 99.5% passing 200 mesh with less than 0.5% above 100 mesh; for ceramic feldspar it is 200 mesh with a controlled residue. Collect in a pulse-jet bag filter with polyester bags; avoid galvanised ducting, which sheds zinc into the product.
Equipment list
| Stage | Equipment | Specification |
|---|---|---|
| Crushing | Jaw crusher, ceramic plates | To 20 mm |
| Iron removal | Permanent magnet, 1,200 gauss | Overband on feed belt |
| Grinding | Ball mill, alumina lined, 2.2 x 7 m | 8 t/h at 325 mesh |
| Classification | Air classifier, ceramic rotor | 200-1250 mesh |
| Collection | Bag filter, stainless ducting | 99.9% at 20 mg/m3 |
| Packing | Valve packer, 25 and 50 kg | Bagged or bulk |
Feldspar is not quartz
Feldspar is softer (Mohs 6 against 7), grinds more easily, and sells on alkali content rather than silica purity. Potash feldspar for ceramics needs K2O above 10% and Na2O below 3%; soda feldspar for glass needs the reverse. The grinding plant is similar but the specification is chemical, which means the beneficiation ahead of the mill — magnetic separation for iron, sometimes flotation to separate feldspar from quartz — matters more than the mill itself.
Questions we are asked before quoting
Can I use a steel-lined mill and still hit glass grade?
No. A steel-lined mill adds 300-600 ppm iron. If the specification is below 150 ppm, the lining has to be ceramic from the first tonne.
What is the practical top fineness?
1250 mesh is achievable but the capacity drops to 10-15% of the 325 mesh rating and power per tonne triples. Above 2500 mesh the material becomes a specialty product with a specialty price.