Kaolin Washing and Refining Line

Reviewed 2026-11-27 Bellian Process Engineering

From raw clay to a 90 brightness paper filler: blunging, grit removal, high-gradient magnetic separation, the brightness leach, and the delamination that adds value.

Kaolin Washing and Refining Line

Kaolin is a deposit business before it is a plant business. Two clays from the same region can differ by ten brightness points, and no amount of processing adds brightness that is not there — it only removes what is obscuring it. A refining plant's job is to take a clay that assays 84 brightness in the ground to a product at 88-90 by removing iron and titania, and to separate the fractions that have different markets.

Capacity50-500 t/d
Brightness85-90 ISO
FinenessBelow 2 micron, 80-95%
Fe2O3Below 0.6%

What the markets buy

MarketBrightnessFinenessKey limit
Paper filler84-8865% below 2 micronBrightness, residue
Paper coating88-9190% below 2 micronViscosity, brightness
Ceramic80-86Residue on 325 mesh lowFired colour, plasticity
Paint and rubber88-92Fineness and oil absorptionBrightness, opacity
Fiberglass and catalyst88-92Controlled PSDChemistry

Process flow

PitBlungerGrit screenHydrocycloneCentrifugeHGMSReductive leachFilter pressDryerMilling

Blunging and dispersion

Raw kaolin at 20-30% moisture is dispersed in water with sodium silicate and soda ash at pH 7-8.5 to a 35-45% solids slip. The dispersion step is critical: an under-dispersed slip cannot be classified, and an over-dosed one will not filter later. The correct dose is measured by the slip viscosity, and it changes with every clay load.

Grit removal and classification

A 325 mesh screen removes the coarse grit, then hydrocyclones cut at 50 micron and disc or decanter centrifuges cut at 2 micron. The coarse fraction (55-70% of the feed) is a ceramic-grade product; the fine fraction (30-45%) is the paper-grade stream. Centrifuge performance decides the split and therefore the revenue mix, so it is the unit that operators watch.

Iron and titania removal

High-gradient magnetic separation at 1.5-2.0 tesla on the fine fraction removes the iron-bearing minerals — hematite, goethite, and the titano-iron oxides that give kaolin its yellow cast. This is where 2-4 brightness points come from. The matrix has to be cleaned every 5-15 minutes with a flush cycle, and the flush water carries 3-8% of the feed as a magnetic reject.

Brightness leaching

A reductive leach with sodium dithionite at pH 3-4 and 40-60 C dissolves the remaining surface iron. The dose is 2-6 kg per tonne of dry clay. Leaching is what takes a magnetically cleaned clay from 86 to 89-90 brightness, and it is the last significant gain available. Above 90 brightness the clay has to be a naturally bright deposit, because oxidation and organic staining cannot be leached out.

Dewatering, drying and milling

Filter press to 60-65% solids, then a rotary dryer or a spray dryer for the coating grades. Spray drying gives spherical agglomerates that disperse well in paper coating colours; rotary drying is cheaper but produces a product that needs more dispersant. Final milling to the target particle size uses a stirred media mill with ceramic media, which also delaminates the booklets and can lift the fine fraction by 10-15%.

Equipment list

StageEquipmentSpecification
DispersionBlunger, 8 m340% solids, pH 7.5
Grit removalVibrating screen 325 meshPlus sand trap
ClassificationHydrocyclone + centrifuge2 micron cut
MagneticHGMS, 2.0 teslaMatrix flush every 10 min
LeachReactor, dithionitepH 3.5, 50 C
DewateringFilter pressTo 62% solids
DryingSpray or rotary dryerBelow 1% moisture
MillingStirred media mill90% below 2 micron

Water is the constraint that gets missed

Kaolin refining consumes 3-6 m3 of water per tonne of product, and the leach effluent is acidic with dissolved iron and manganese. A closed circuit with a thickener, a filter press and pH neutralisation is not optional in most jurisdictions. The water circuit is typically 20-25% of the plant capital, and projects that budget it at 5% run out of money before commissioning.

Questions we are asked before quoting

Can I raise brightness by 8 points?

Typically 3-6 points from magnetic separation and leaching combined. Above that you need a brighter deposit, or a bleaching route with ozone or a stronger reductant that costs more than the price premium.

What is the difference between filler and coating grade?

Fineness and viscosity. Coating needs 90% below 2 micron with a narrow distribution and a controlled shape; filler is coarser and much less demanding.

Other solution categories

Same engineering team, different process route.

Send your material. We will send the flow sheet.

Feed size, moisture, target capacity and product spec are enough to start. Quotations and plant layouts are free and usually back within one working day.

Request a flow sheet WhatsApp us