Heavy Mineral Sand Processing (Titanium and Zircon)
Beach sand route combining gravity, magnetic and electrostatic separation to split ilmenite, rutile, zircon and monazite from a 2-8% heavy mineral feed.

Mineral sands are a sorting problem rather than a size-reduction problem. The valuable minerals — ilmenite, rutile, zircon, leucoxene, monazite — are already liberated by the sea, and the plant's job is to separate them from each other using the small differences in density, magnetic susceptibility and electrical conductivity that distinguish them. Nothing is crushed. Everything is sorted.
Four properties, four separators
Every mineral in a heavy mineral suite has a distinct fingerprint: density, magnetic response at a given field strength, and conductivity when charged. The plant is a cascade that exploits them in order, cheapest first.
| Mineral | Density | Magnetic | Conductive |
|---|---|---|---|
| Ilmenite | 4.7 | Strongly, at 0.3-0.6 T | Yes |
| Leucoxene | 4.2 | Weakly, above 1.0 T | Yes |
| Rutile | 4.2 | Non-magnetic | Yes |
| Zircon | 4.6 | Non-magnetic | No |
| Monazite | 5.0 | Weakly, 1.2 T | No |
| Quartz | 2.65 | Non-magnetic | No |
Process flow
Wet concentration
Feed is screened at 1 mm and the minus 1 mm slurry goes to spiral concentrators, which reject 92-98% of the mass as light sand. Spirals work because the density difference is large and the feed is already fine; two stages of spirals bring the heavy mineral content to 60-90%.
Magnetic separation
The dried heavy concentrate runs through a low-intensity magnetic separator at 0.3 T, which pulls out magnetite and any tramp iron. Then a high-intensity induced roll at 1.0-1.5 T splits ilmenite from rutile and zircon. Multiple passes at increasing field strength separate ilmenite, then leucoxene, then monazite.
Electrostatic separation
The non-magnetic fraction goes to a high-tension roll separator. Rutile is conductive and is thrown off the roll; zircon is non-conductive and stays on the belt until brushed off. This is the only practical way to separate rutile from zircon, whose densities are too close for gravity.
Equipment list
| Stage | Equipment | Function |
|---|---|---|
| Wet plant | 1 mm wet screen + 24 spiral starts | Reject 95% light sand |
| Cleaner spirals | 12 starts | Heavy mineral to 70% |
| Dryer | Rotary dryer | Below 0.5% moisture |
| LIMS | Rare earth roll, 0.3 T | Magnetite removal |
| HIMS | Induced roll, 1.0-1.5 T, 3 passes | Ilmenite, leucoxene, monazite |
| HTS | High-tension roll, 25 kV | Rutile / zircon split |
| Dewatering | Product thickeners | Separate product streams |
The dry plant is where the value is
The wet plant is cheap and robust; the dry plant is where grade is made and where most operating problems occur. Electrostatic separation needs the feed at below 0.5% moisture and at a controlled temperature, because surface moisture changes conductivity completely. A mineral sand plant that runs well on a dry day and badly after rain is a dryer problem, not a separator problem.
Questions we are asked before quoting
Can I do this without a wet plant?
No. Dry separation on raw beach sand cannot handle the 95%+ non-heavy fraction; the equipment would be enormous. The wet spiral stage is what makes the dry plant small enough to be economic.
What about monazite and radiation?
Monazite carries thorium and uranium and is radioactive. Above about 1% monazite in the feed the plant needs radiation monitoring, sealed areas and a licensed disposal route for the monazite stream. This is a permitting issue that often decides project viability.
Other solution categories
Same engineering team, different process route.