Tin Ore Gravity Concentration Line

Reviewed 2026-11-27 Bellian Process Engineering

Cassiterite recovery by multistage gravity: jigs, spirals and shaking tables bring a 0.3-1.5% Sn feed to 60-70% Sn concentrate, with sulphide flotation for cleanup.

Tin Ore Gravity Concentration Line

Tin is a gravity mineral, and almost every tin concentrator in the world works on that principle. Cassiterite has a specific gravity of 6.8-7.0 against 2.65 for quartz, a ratio large enough that a well-run gravity circuit reaches 85-90% recovery. Where tin plants fail is on the fine end: below 40 microns gravity stops working and the tin goes out with the tailings.

Capacity100-1,000 t/d
Feed grade0.3-1.5% Sn
Concentrate60-70% Sn
Recovery80-88%

Multistage gravity, because no single device covers the range

Cassiterite arrives in a size range from 20 mm down to a few microns, and no single gravity device handles that span. The standard circuit therefore runs three devices in series by size: a jig for 2-20 mm, spirals for 0.1-2 mm, and tables for 0.04-0.1 mm. Each device treats the size band where it is efficient and sends the rest on.

Size bandDeviceTypical recovery
2-20 mmJig85-92%
0.1-2 mmSpiral concentrator80-88%
0.04-0.1 mmShaking table70-80%
Below 0.04 mmCentrifugal / slime table45-65%

Process flow

CrushingWashing + screeningJigGrindingSpiralTableSulphide flotationMagnetic cleanup

Crushing and jigging

Crush to 20 mm in a jaw crusher and a roll crusher, then jig the 2-20 mm fraction. On rich ore the jig alone can produce a saleable 40-50% Sn concentrate and reject 60% of the mass before any grinding, which is where the operating cost is saved.

Grinding and fine gravity

Jig tail is ground in a Ball Mill to 2 mm, then classified. Spirals take 0.1-2 mm; tables take the fines. The grind size is set by liberation, and tin ores are usually well liberated at 0.5 mm, which is coarse enough that slime losses stay manageable.

Concentrate cleanup

Gravity concentrate contains cassiterite plus sulphides (pyrite, arsenopyrite) and often wolframite. Sulphide flotation with xanthate at pH 5 removes the sulphides, then a magnetic pass removes wolframite and magnetite. Final concentrate 60-70% Sn, with arsenic below 0.5% for smelter acceptance.

Equipment list

StageEquipmentNote
CrushingJaw + double roll to 20 mmMinimise fines
Jig2-chamber jig, 2-20 mmReject 60% early
GrindingBall mill 1,500 x 3,000To 2 mm
Spiral12 starts, 0.1-2 mmRougher
Table6 shaking tablesCleaner and fines
Flotation4 cells, sulphide removalpH 5, xanthate
MagneticDry induced roll, 1.2 TRemove wolframite

The arsenic and sulphur limits

Smelters reject tin concentrate above 0.5% As and about 1% S. Both come from sulphides that gravity concentrates along with cassiterite because pyrite has a density of 5.0, not far below cassiterite. That is why the flotation cleanup stage is not optional, and why a plant that skips it ends up with a concentrate nobody will buy.

Questions we are asked before quoting

Can I recover tin from old tailings?

Often yes, and it can be very profitable. Old gravity tailings typically still carry 0.1-0.3% Sn in the fine fraction, which modern centrifugal concentrators recover where the original plant could not.

What is the water requirement?

6-10 m3 per tonne of feed. A closed circuit with a thickener brings makeup down to 1-2 m3.

Other solution categories

Same engineering team, different process route.

Send your material. We will send the flow sheet.

Feed size, moisture, target capacity and product spec are enough to start. Quotations and plant layouts are free and usually back within one working day.

Request a flow sheet WhatsApp us