Tungsten Ore Processing Line (Wolframite and Scheelite)

Reviewed 2026-11-27 Bellian Process Engineering

Two different routes for the two tungsten minerals: gravity and magnetic separation for wolframite, heated flotation for scheelite, both reaching 65% WO3 concentrate.

Tungsten Ore Processing Line (Wolframite and Scheelite)

Tungsten is two ores wearing one name. Wolframite is dense (7.1-7.5) and weakly magnetic, so gravity and magnetic separation do the work. Scheelite is dense (6.1) but not magnetic, and it floats readily with fatty acids — which is convenient until you need to separate it from calcite and fluorite, which also float. A plant designed for one will not treat the other.

Capacity50-500 t/d
Feed grade0.2-1.5% WO3
Concentrate65% WO3
Recovery70-85%

Wolframite: gravity and magnetics

The density difference against quartz (2.65) is so large that gravity does most of the work. The circuit is multistage: jigs on the coarse fraction, shaking tables on the middlings, and a final magnetic separation to pull wolframite away from cassiterite and sulphides, which gravity cannot separate because their densities are too close.

Process flow (wolframite)

CrushingGrindingJigShaking tableMagnetic separationGravity concentrate

Grinding, and the slime problem

Wolframite is brittle and slimes easily below 75 microns, and slime tungsten is lost. The circuit grinds to 2 mm first, runs a jig, and only grinds the jig tail further. This "grind as little as possible" discipline is what separates a 75% recovery plant from a 55% one.

Table and magnetic cleanup

Shaking tables produce a rough concentrate at 20-40% WO3. A dry magnetic separator at 1.0-1.3 T then removes the magnetic fraction (wolframite is weakly magnetic; cassiterite and pyrite are handled differently). Final concentrate reaches 65-70% WO3 after cleaning.

Scheelite: flotation with a heated step

Scheelite floats with sodium oleate at pH 9-10, but so do calcite, fluorite and apatite. The standard solution is Petrov's method: heat the rougher concentrate to 90 C with sodium silicate for 30-60 minutes, which desorbs the collector from the gangue minerals but not from scheelite, then re-float. It is slow, energy-intensive, and still the most reliable method in use.

StageReagentDoseFunction
RougherSodium carbonate1-2 kg/tpH 9-10, dispersant
RougherSodium silicate2-5 kg/tDepress silicates
RougherSodium oleate200-500 g/tCollector
Heated cleanerSodium silicate at 90 C10-20 kg/tDesorb gangue minerals

Equipment list

RouteEquipmentFunction
CrushingJaw + roll crusher to 5 mmMinimise fines
Wolframite gravityJig + 6 shaking tablesRough concentrate
Wolframite magneticsDry induced roll, 1.2 TWolframite / cassiterite split
Scheelite flotation6 rougher + 4 cleaner cellsFatty acid flotation
Heated conditioningSteam-heated tanks, 90 CPetrov process
DewateringFilter pressConcentrate cake

Questions we are asked before quoting

Can one plant treat both minerals?

Yes, but as two parallel circuits sharing crushing and dewatering. The gravity section and the flotation section cannot be merged because the size ranges and the chemistry conflict.

Why is my recovery stuck at 60%?

Usually over-grinding producing minus 20 micron slime that gravity cannot catch. Add a slime table or a centrifugal concentrator on the overflow before it goes to tails.

Other solution categories

Same engineering team, different process route.

Send your material. We will send the flow sheet.

Feed size, moisture, target capacity and product spec are enough to start. Quotations and plant layouts are free and usually back within one working day.

Request a flow sheet WhatsApp us