Hematite Beneficiation Line
Hematite is only weakly magnetic, so the route combines gravity, high-gradient magnetic separation and reverse flotation to reach 62-66% Fe from a 30-45% feed.

Hematite has a magnetic susceptibility roughly two orders of magnitude lower than magnetite, which means the simple drum separator that works beautifully on magnetite will not hold it. The industry answer is a combination: gravity for the coarse fraction, high-gradient magnetic separation for the fine fraction, and reverse flotation when silica has to come out.
Why the circuit is more complex
Hematite is often finely disseminated and often associated with quartz in a banded structure. Liberation is rarely complete above 50 microns, so the plant has to grind fine and then recover from a slurry that is hard to separate. Each of the three techniques available has a size range where it works, and the circuit is arranged so that each particle sees the technique suited to its size.
| Technique | Effective size range | Use in a hematite plant |
|---|---|---|
| Gravity (jig, spiral) | 0.1-10 mm | Coarse pre-concentration, reject 30-50% |
| High-gradient magnetic (SLon) | 10-200 micron | Main concentration and slime recovery |
| Reverse flotation | 20-150 micron | Silica removal for premium concentrate |
Process flow
Gravity stage
A jig on the 2-10 mm fraction and spirals on the 0.1-2 mm fraction reject 30-50% of the mass as coarse tailings at very low cost. This is done before fine grinding, and it is the reason a hematite plant can compete on operating cost with a magnetite plant despite the more complex downstream circuit.
High-gradient magnetic separation
A pulsating high-gradient magnetic separator with a 1.5-2.0 T background field, using a 1-3 mm steel matrix. The pulsation is the key detail: it stops the matrix from blinding with fine particles, which is what limits conventional HGMS throughput. Recovery on the 10-74 micron fraction reaches 80-85%.
Reverse flotation
When the concentrate has to go above 64% Fe, an amine collector floats quartz off the iron at pH 10-10.5, with starch depressing the hematite. This is the only way to get below 4% SiO2 on finely disseminated ore.
Equipment list
| Stage | Equipment | Note |
|---|---|---|
| Crushing | Jaw + cone to 10 mm | Two stage |
| Grinding | Ball Mill 2,700 x 4,500 + cyclones | 80% passing 75 micron |
| Gravity | Jig + 12 spiral starts | Reject 30-50% coarse tails |
| HGMS | SLon-1500 pulsating vertical ring | 1.5-2.0 T, steel matrix |
| Flotation | 6 rougher + 4 cleaner cells | Amine collector, starch depressant |
| Dewatering | 15 m thickener + filter press | 8-9% moisture |
Operating cost reality
High-gradient magnetic separation is power-hungry: 1.5-2.5 kWh per tonne of feed just for the magnet, on top of grinding. A 1,000 t/d hematite plant running gravity plus HGMS draws 55-65 kWh per tonne of concentrate, against 35-45 for an equivalent magnetite plant. That is why hematite projects are more sensitive to the iron price than magnetite ones.
Questions we are asked before quoting
Can I just use a strong drum magnet?
No. A drum at 3,000 gauss will recover coarse hematite but loses 40-60% of the fine fraction. HGMS with pulsation is the only practical route for fines.
Is roasting worth it?
Magnetising roasting converts hematite to magnetite and lets you use cheap magnetic separation, but it needs 750-800 C and 30-50 kg of coal per tonne. It is only economic for ores that respond poorly to everything else, and only at scale above 1,000 t/d.
Other solution categories
Same engineering team, different process route.