Bauxite Washing and Beneficiation Line
Reactive silica is what makes bauxite expensive to refine. Scrubbing, screening and desliming to lift the alumina-to-silica ratio before the Bayer circuit sees the ore.

Bauxite is not sold on alumina content alone. A refinery buying ore at 55% Al2O3 with 4% reactive silica loses more soda in the digestion circuit than it saves on the ore price. The metric that governs the transaction is the alumina-to-silica ratio, and washing is the cheapest way to move it: 60-75% of the reactive silica in a typical diasporic bauxite sits in the clay fraction below 1 mm, which can be removed with water and a screen.
What the refinery actually penalises
| Component | Typical run-of-mine | Saleable target | Why |
|---|---|---|---|
| Al2O3 | 50-60% | Above 55% | Yield per tonne of ore |
| Reactive SiO2 | 4-9% | Below 4% | Each 1% consumes 10-15 kg soda per tonne |
| Fe2O3 | 5-25% | Below 20% | Red mud volume and disposal cost |
| Moisture | 8-15% | Below 10% | Freight is paid on water |
The A/S ratio is the shorthand: Al2O3 divided by reactive SiO2. Below 7 the Bayer process becomes uneconomic for most refineries; above 10 the ore commands a premium. Washing typically lifts the ratio by 1.5-3 points, which is often the difference between a sellable and an unsellable ore.
Process flow
Scrubbing is the key unit
Bauxite clay does not disperse in a simple wash. An attrition scrubber at 40-60% solids with 8-12 minutes residence breaks the clay coating off the pisolitic nodules, which is what releases the silica into the fine fraction. A plant without a scrubber and with only a spray screen recovers 20-30% of the available silica reduction; with a scrubber it recovers 55-70%.
Screening and desliming
A wet vibrating screen at 1-2 mm separates the washed coarse product from the clay slurry. The cut point matters: a 1 mm cut removes more silica but loses more alumina fines with it. Most operations run at 1.5 mm and accept 3-5% alumina loss to the tailings.
Water and tailings
Washing consumes 1.5-3 m3 of water per tonne of ore, and the resulting slime is the hardest part of the plant to permit. A thickener with high-rate flocculation plus a filter press returns 85-90% of the water and produces a stackable cake. Red mud from the refinery is a separate problem, but the washery slime is often the first environmental objection to a new mine.
Equipment list
| Stage | Equipment | Specification |
|---|---|---|
| Feeding | Apron feeder + grizzly | 800 t/d, 600 mm lumps |
| Crushing | Roll crusher or sizer | To 100 mm |
| Scrubbing | Attrition scrubber 2.4 m | 8-12 minutes residence |
| Screening | Wet vibrating screen | 1.5 mm cut |
| Classification | Hydrocyclone cluster | 75 micron overflow |
| Dewatering | Dewatering screen + thickener | Product below 12% moisture |
| Water | Filter press on tails | 85-90% recovery |
When washing is not enough
For high-silica diasporic ores the clay fraction is only part of the problem — the silica is also locked inside the nodules as kaolinite inclusions and as aluminosilicate in the matrix. Two further routes exist. Magnetic separation removes iron-bearing minerals but does little for silica. Flotation of the diaspore from kaolinite with a collector at pH 9-10 works in the laboratory and has been piloted at scale, but the reagent cost is high and the selectivity is sensitive to the ore. For most operations the practical answer is selective mining and blending rather than a complex concentrator.
Questions we are asked before quoting
Can I wash bauxite without a scrubber?
You can, and you will remove 20-30% of the silica instead of 60%. If the ore already meets the refinery's ratio, no scrubber is needed; if it does not, the scrubber is the plant.
What moisture does the product need?
Below 10% for sea freight, because the cargo liquefaction risk above that is a shipping hazard, not just a cost issue. Most contracts specify a transportable moisture limit and test it every shipment.
Other solution categories
Same engineering team, different process route.