Nickel Laterite Ore Preparation Line
Laterite ore at 30-35% moisture, 1.5-2.2% nickel, and two very different routes: RKEF smelting needs dry lump, HPAL needs fine slurry. The preparation plant decides which one is possible.

Nickel laterite is a wet, sticky, low-grade ore and almost all of its processing cost is decided before the metallurgical plant. The ore comes out of a tropical pit at 30-35% moisture with a clay fraction that blinds screens and plugs chutes. Two industrial routes consume it — rotary kiln electric furnace smelting, which needs dry and sized feed, and high-pressure acid leach, which needs a fine slurry — and they impose opposite requirements on the preparation plant.
Two ore types in one deposit
| Horizon | Ni | Fe | MgO | Route |
|---|---|---|---|---|
| Limonite (upper) | 1.2-1.6% | 40-50% | 2-5% | HPAL, or iron-nickel |
| Saprolite (lower) | 1.8-2.5% | 12-20% | 15-25% | RKEF smelting |
The two horizons need to be mined and stockpiled separately. Blending them and feeding a single stream to the smelter is the most common and most expensive mistake in a laterite operation: the saprolite needs high temperature and the limonite generates too much slag, and the furnace responds by running badly on both.
Process flow
Crushing in sticky ore
Laterite at 32% moisture does not flow through a jaw crusher; it packs. The usual solution is a single-roll or mineral sizer with a toothed rotor that tears rather than compresses, or a jaw crusher with a specially profiled chamber and a vibrating feeder that keeps the material moving. Washing the feed with high-pressure water before crushing converts the problem into a slurry problem, which is easier but adds water treatment.
Screening at high moisture
A conventional vibrating screen blinds within hours on laterite. Wet screening with spray water at 1-2 mm works; dry screening only works below 20% moisture. Some plants use a trommel with internal water sprays, which tolerates sticky feed better than a flat deck because the rotation keeps the apertures clear.
Drying for RKEF
A rotary dryer at 400-500 C inlet gas brings the ore from 32% to 18-20%, which is the feed condition for a rotary kiln. Drying below 15% is not necessary and costs fuel, because the kiln will drive off the balance anyway. Laterite dryers are large — a 5,000 t/d operation needs a 4 x 32 m dryer — and they are the single largest fuel consumer in the preparation plant.
Equipment list
| Stage | Equipment | Specification |
|---|---|---|
| Feeding | Apron feeder with variable speed | 2,000 t/d |
| Crushing | Mineral sizer, toothed | To 150 mm, sticky duty |
| Screening | Trommel with water sprays | 2 mm cut, 60% solids |
| Dewatering | Dewatering screen | To 25% moisture |
| Drying | Rotary dryer 4 x 32 m | To 18-20% moisture |
| Dust and fume | Bag filter, cyclone | Dryer exhaust |
| Stockpile | Covered shed | Rain adds 3-5% moisture |
The moisture that is invisible on the specification
Laterite in a tropical stockpile gains 3-5% moisture in a single monsoon week. A dryer sized on the annual average will be the bottleneck for four months a year, and a smelter that receives wet ore cuts its feed rate to protect the kiln. Size the dryer on the wet-season moisture, not the annual mean; the capital difference is 15% and the production difference is 20%.
Questions we are asked before quoting
Can the same plant feed RKEF and HPAL?
Only the mining and stockpiling can be shared. RKEF needs dry sized lump and HPAL needs a slurry ground below 1 mm, which are different circuits.
What nickel grade makes laterite viable?
Above 1.8% for RKEF at current energy prices, above 1.2% for HPAL where the cobalt credit helps. Below 1.2% the ore is a construction material, not an ore.
Other solution categories
Same engineering team, different process route.