Henan Bellian Mining Machinery
Home/ Solutions/ Mineral Processing/ Process route
Mineral Processing · Process route

Graphite Flotation and Purification Line

Reviewed 2026-11-27 Bellian Process Engineering

Flake graphite is sold on carbon content and flake size, and the two fight each other. Multi-stage flotation, the regrind that lifts grade, and chemical purification above 99%.

Graphite Flotation and Purification Line

Graphite is the easiest mineral in this book to float and the hardest to float well. Natural flake graphite is strongly hydrophobic, so a rougher with kerosene and a frother recovers 90% of it in four minutes. But the market buys two things at once: carbon content above 94-99% and flake size above 80-150 mesh, and every regrind that raises the grade breaks the flakes that give the product its value. The circuit is a negotiation between those two numbers.

Capacity50-500 t/d
Carbon85-99.9%
Flake size80-325 mesh
Recovery85-92%

The grade-size trade-off, quantified

ProductCarbonFlake sizeRelative value
Large flake94-97%Above 80 mesh (+180 micron)100
Medium flake94-97%80-150 mesh70-80
Fine flake90-95%150-325 mesh40-55
Amorphous or fines80-90%Below 325 mesh20-30
Spherical purified99.95%10-20 micron400-800

A plant that grinds everything to 325 mesh to hit 95% carbon has destroyed 60% of the value of the ore. The correct approach is staged liberation: float coarse, clean coarse, and regrind only the fractions that need it.

Process flow

Run-of-mineJaw crusherRod millRougher flotationScreenRegrindCleaner flotationDewateringDrying

Crushing and coarse grinding

Flake graphite must not be crushed in a way that breaks the flakes. A jaw crusher to 25 mm followed by a rod mill is standard; a hammer mill or an impact crusher will shatter the flakes and the loss shows up as a lower proportion of plus-100 mesh in the final product. Rod mill discharge at 0.5-1 mm is the usual target for the rougher.

Rougher flotation

Kerosene at 100-300 g/t as collector, pine oil or MIBC as frother, pH 7-8, 25-30% solids, 4-6 minutes. The rougher produces a 60-75% carbon concentrate at 90-95% recovery. Flotation is fast because graphite is naturally hydrophobic; the challenge is selectivity against the mica and quartz that report with it.

Cleaning and regrinding

Five to eight cleaning stages are normal, with regrinding between stages 2 and 4. Each cleaning stage lifts the grade by 5-10 points; the first three are cheap and the last three are expensive because they operate on a small tonnage. The intermediate size fractions — the ones that are neither coarse enough to sell as flake nor fine enough to pass as fines — are the ones that get reground.

Drying

Filter cake at 15-20% moisture goes to a rotary dryer at 200-300 C, or to a flash dryer for fine product. Graphite is a good thermal conductor and dries quickly, but the dried powder is extremely dusty and requires enclosed conveying and a well-sized bag filter.

Equipment list

StageEquipmentSpecification
PrimaryJaw crusherTo 25 mm, gentle
GrindingRod mill 1.5 x 3.0 mTo 0.5 mm
RougherFlotation, 8 m3 cellsKerosene + MIBC
ClassificationScreen, 80 and 150 meshSplits flake grades
RegrindBall Mill, smallIntermediate fractions only
Cleaners6 stages, column or conventionalTo 95% carbon
DewateringFilter + rotary dryerBelow 1% moisture

Above 99%: chemical purification

Flotation stops at 95-97% carbon because the remaining impurity is locked inside the flakes. Two routes take it further. Alkali roasting with sodium hydroxide at 500-700 C dissolves the silicates and is followed by washing and acid leaching, reaching 99-99.5%. Hydrofluoric acid leaching reaches 99.9% but is a serious safety and permitting matter. For battery anode material the requirement is 99.95% with a controlled particle size, which is a chemical plant with a grinding circuit attached, not a flotation plant.

Questions we are asked before quoting

What flake size should I target?

Whatever the ore will give without regrinding. Test the size distribution of the rougher concentrate first; a deposit that is naturally 60% below 150 mesh will never produce a large-flake premium product.

Can I float graphite and sulphides together?

No. Sulphide flotation uses different reagents and pH and will contaminate the graphite concentrate. Float the sulphides first with xanthate at pH 9, then graphite.

Other solution categories

Same engineering team, different process route.

Send your material. We will send the flow sheet.

Feed size, moisture, target capacity and product spec are enough to start. Quotations and plant layouts are free and usually back within one working day.

Request a flow sheet WhatsApp us